Low-Alloy Steels Manual Electrode E7018-C2L HEC - tria, Haiyang MSR filum coil glutino
Praecipua compositio est 3.5% Ni chalybe, humilis hydrogenii potassii genus manu virgae glutino, ad -100°C temperatura operans, ejus liquefactio metalli obductis ictum durities est optimum
Arcus stabilis, fundendi minus, corona bona, remotio scoria facilis
X Ray perficientur est optimum
CHEMICAL COMPONET:
ADMISSUS (wt%) | C | Si | Mn | P | S | Ni | Cr | Mo | Other | |
GB/T REGULAE | 0.093 | 0.18 | 0.66 | 0.004 | 0.003 | 3.58 | 0.031 | 0.009 | - |
MACHINA proprietas:
POSSESSIO | VICTORITAS (MPa) | PROLATIO VIS (MPa) | Prolongatio(%) | IMAPACT VALEO J/℃ | Caloris curatio ° C * h * | |||||
GB/T REGULAE | 485 | 565 | 27 | 67/-100 | 620*1 |
PARAMETERS WELDING RECOMMENDED:
DIAMETERS SPECIFICATIONS(mm) | 2.6*350 | 3.2*350 | 4.0*400 | 5.0*400 | |||||
ELECTRICITY (Amp) | H/W | 70-100 | 100-140 | 140-180 | 180-230 | ||||
O/W* | 60-90 | 90-130 | 120-160 | - |
Sino-russicus ante orientem
Haiyang nuclei potentia Planta
-
400,000 millia talentorum ore carrier
CHEMICAL COMPONET:
ADMISSUS (wt%) | C | Si | Mn | P | S | Ni | Cr | Mo | Other | |
GB/T REGULAE | 0.093 | 0.18 | 0.66 | 0.004 | 0.003 | 3.58 | 0.031 | 0.009 | - |
MACHINA proprietas:
POSSESSIO | VICTORITAS (MPa) | PROLATIO VIS (MPa) | Prolongatio(%) | IMAPACT VALEO J/℃ | Caloris curatio ° C * h * | |||||
GB/T REGULAE | 485 | 565 | 27 | 67/-100 | 620*1 |
PARAMETERS WELDING RECOMMENDED:
DIAMETERS SPECIFICATIONS(mm) | 2.6*350 | 3.2*350 | 4.0*400 | 5.0*400 | |||||
ELECTRICITY (Amp) | H/W | 70-100 | 100-140 | 140-180 | 180-230 | ||||
O/W* | 60-90 | 90-130 | 120-160 | - |